Neutral salt spray to ASTM B117 for 24, 48 or 96 hours tells you one thing: how the plating and the housing resist a continuous 5% salt fog at 35 °C. It does not predict field life in a coastal installation, because real failures are driven by sulphur, humidity cycling and galvanic coupling, not by constant fog.

It is still worth specifying, because it is reproducible and it catches gross plating defects. It just should not be the only corrosion test on the drawing.

What the common durations mean

Duration Typical result on a plated connector Interpretation
24 h No red rust on gold parts Basic plating integrity
48 h Tin tails show white corrosion, no red rust Acceptable for indoor
96 h Tin may show red rust at edges Not a failure for tin; it is expected
240 h+ Only meaningful with a stated acceptance criterion Marine or outdoor claims

Note the tin commentary. Tin corrodes in salt spray by design; the corrosion product is white and mildly protective. A buyer who rejects a tin part for white corrosion at 48 hours is rejecting normal behaviour.

The three things salt spray misses

Sulphur. Industrial and urban air contains sulphur compounds that attack silver and thin gold through pores. Salt spray has no sulphur in it, so a part can pass 96 hours and still fail in a city in two years.

Humidity cycling. Real cabinets go from 20 °C to 60 °C daily. That cycling pumps moisture into crevices and drives galvanic corrosion between dissimilar platings. Constant fog does not reproduce it.

Fretting. Vibration moves the contact by microns, wears the plating and produces oxide debris. A static salt spray test has no movement at all.

What to specify instead, or as well

  • Mixed flowing gas (ASTM B845, class 2 or 3) for telecom and industrial cabinets. It includes H₂S and reproduces pore corrosion.
  • Thermal cycling with humidity for outdoor enclosures.
  • Fretting or vibration plus low-signal resistance for anything on a machine.
  • Salt spray only when the requirement is genuinely marine and the customer asks for it.

For most industrial customers we run salt spray because it is on the drawing, and we would rather discuss mixed flowing gas than add hours to a test that does not correlate.

Reading a report properly

Check the standard, the duration, whether the sample was mated or unmated, whether it was cleaned before inspection, and the acceptance criterion. A report that says "48 h salt spray passed" without those four items is not reproducible, and you cannot compare it to another supplier’s report.

Does gold plating pass salt spray?

Gold itself does, but thin gold is porous. At 3 µin the pores let the fog reach the nickel, and the result depends on the underplate. At 10 µin and above, a 48-hour pass is routine.

Is 96 hours better than 48?

Only if the acceptance criterion is meaningful. Doubling the hours on a test that does not correlate with your environment buys paperwork, not reliability.

Do housings need salt spray testing?

Plastic does not corrode, so the test is about the metal parts. A housing test is only relevant for metal shells or shielding cans.

Tell us the installation environment and we will suggest a test that correlates with it, and quote the plating that passes. See our quality process and the plating thickness guide.