Choose the housing by the soldering process. Reflow at 260 °C peak needs PA6T, PA9T or LCP. Wave solder at 260 °C for a few seconds is fine with PBT. Hand soldering is fine with all four. Everything else, including the HDT on the datasheet, is a tiebreaker.
The datasheet comparison is misleading because heat deflection temperature is measured under a standard load, not under the thermal shock of a reflow oven with a 40-pin body acting as a heat sink.
The four materials in practice
| Material | HDT | Reflow | Relative cost | Best for |
|---|---|---|---|---|
| PBT | 200–210 °C | No | Low | Wave solder, through-hole, cost-driven |
| PA6T | ~290 °C | Yes | Medium | General SMT headers |
| PA9T | ~265 °C | Yes | Medium-high | Low moisture absorption, fine pitch |
| LCP | 280–340 °C | Yes | High | Thin walls, 1.27 mm and finer |
Why PBT fails in reflow
PBT softens near 200 °C. In a reflow oven the body does not melt, it sags. On a 2×5 header the sag is invisible and the part works. On a 2×20 header the middle of the body bows, the tails lift, and the joints open.
You will not see it at AOI on the top side. You will see it as a unit that fails functional test intermittently, and then works when you press on the connector.
Moisture and popcorning
Polyamides absorb moisture from the air. A reel that sat in a humid warehouse for a month will release that moisture as steam in the oven, which shows up as bubbles on the body or a hairline crack at the pin exit.
- Keep PA6T and PA9T reels sealed until use; use them within the stated floor life.
- PBT absorbs less and is more forgiving in storage.
- LCP absorbs least and is the safest choice for a line with poor humidity control.
If a customer reports "cracked housings after reflow" and the parts were fine at incoming inspection, moisture is the first thing to check, not the material grade.
Flammability and the file number
All four are available in UL94V-0. The rating is only meaningful with the file number and the thickness it applies to, so a drawing that says "UL94V-0" and nothing else is not a specification. Ask for the yellow card reference and check the wall thickness on it matches your part.
Can I use PA6T for wave solder?
Yes, it is over-specified but harmless. The cost difference per part is small; the reason to choose PBT is price, not process.
Does colour affect the material?
Black is standard and cheapest. Natural and white grades exist but the pigment can change the crystallization and the warpage on long bodies. Test the colour you intend to ship.
Is LCP always better?
No. LCP is stiffer and more dimensionally stable, but it is brittle at the pin exit and costs more. Use it where the wall is thin or the pitch is fine, not as a default upgrade. See where LCP earns its cost.
Tell us the soldering process and the body length and we will recommend the material that survives it without paying for headroom you do not need. Housings in all four materials are quoted from our molding capability.